Grade GX25CrNiSi20-14
Germany W-Nr. 1.4832
Corresponding Standard DIN EN 10295-2003
Heat Resistant Steel Castings
Classification Cast Steel
Density 7.8 g/cm3
GX25CrNiSi20-14 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu * Mo W * V * Nb * Co *
Minimum Value 0.15 0.5 - - - 19 13 - - - - - -
Maximum Value 0.35 2.5 2 0.04 0.03 21 15 0.25 0.5 0.6 0.12 0.6 1
GX25CrNiSi20-14 Mechanical Properties
condition Test Temperature Tensile Strength
σb
Mpa
Specified Plastic Yield Strength
Rp0.2
Mpa
Elongation or Extension Rate
δ
%
cast steel Room Temperature ≥450 ≥230 ≥10
cast steel 600°C Creep Strength for 1%-10000h
82
cast steel 700°C Creep Strength for 1%-10000h
46
cast steel 800°C Creep Strength for 1%-10000h
23
cast steel 900°C Creep Strength for 1%-10000h
10
Approximate Comparison Table Heat-Resistant Cast Steels and Alloys
China Japan International Organization for Standardization Germany France Russia United Kingdom
GB ISC JIS ISO DIN EN/DIN W-Nr. NF EN/NF GOST BS EN/BS
ZG25Cr20Ni14Si2 C53821 SCH 32 GX25CrNiSi20-14 GX25CrNiSi20-14 1.4832 GX25CrNiSi20-14 20Х20Н14С2Л GX25CrNiSi20-14
GX25CrNiSi20-14 Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!