Grade GX40CrNiSi27-4
Germany W-Nr. 1.4823
Corresponding Standard DIN EN 10295-2003
Heat Resistant Steel Castings
Classification Cast Steel
Density 7.6 g/cm3
GX40CrNiSi27-4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu * Mo W * V * Nb * Co *
Minimum Value 0.3 1 - - - 25 3 - - - - - -
Maximum Value 0.5 2.5 1.5 0.04 0.03 28 6 0.2 0.5 0.2 0.08 0.2 0.5
GX40CrNiSi27-4 Mechanical Properties
condition Test Temperature Tensile Strength
σb
Mpa
Specified Plastic Yield Strength
Rp0.2
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
cast steel Room Temperature ≥550 ≥250 ≥3 Agreed annealing hardness Max.
cast steel 600°C 100h (1000h) Rupture Strength σr 100(80) Creep Strength for 1%-10000h
28
cast steel 700°C 100h Rupture Strength σr
45
Creep Strength for 1%-10000h
15
cast steel 800°C 100h Rupture Strength σr
25
Creep Strength for 1%-10000h
8
cast steel 900°C 100h (1000h) Rupture Strength σr 15(5) Creep Strength for 1%-10000h
4
cast steel 1000°C Creep Strength for 1%-10000h
1
1 Approximate Comparison Table Heat-Resistant Cast Steels and Alloys
China Taiwan, China Japan South Korea United States International Organization for Standardization Germany France United Kingdom
GB ISC CNS JIS KS ASTM UNS ISO DIN EN/DIN W-Nr. NF EN/NF BS EN/BS
ZG40Cr27Ni4Si2 C54890 SCH 11 SCH 11X HRSC 11 HD J93005 GX40CrNiSi27-4 GX40CrNiSi27-4 1.4823 Z30CN26.05M GX40CrNiSi27-4
2 Approximate Comparison Table Heat-Resistant Cast Steels and Alloys
China Japan United States Germany United Kingdom
GB JIS ASTM UNS DIN EN/DIN W-Nr. BS EN/BS
ZG5Cr25Ni2 SCH2 HC J92605 G-X40CrNi24 5 1.4822
1.4823
452C11
GX40CrNiSi27-4 Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!