Grade S275ML
Corresponding Standard ISO 630-3-2021
Structural Steels — Part 3: Technical Delivery Conditions for Fine-Grain Structural Steels
Classification Alloy Steel
S275ML Chemical Element Composition Content (%)
Component C Si Mn P S ①② Cr Ni Cu Mo N Ti V Nb Al
Minimum Value - - - - - - - - - - - - - 0.02
Maximum Value 0.13 0.5 1.5 0.025 0.02 0.3 0.3 0.55 0.1 0.015 0.05 0.08 0.05 -
S275ML Mechanical Properties
thickness
t
mm
Test Temperature Tensile Strength
σb
Mpa
Specified Plastic Yield Strength
Rp0.2
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
t≤16 room temperature 370~530 ReH: ≥275 ≥24
16<t≤40 370~530 ReH: ≥265 ≥24
40<t≤63 360~520 ReH: ≥255 ≥24
63<t≤80 350~510 ReH: ≥245 ≥24
80<t≤100 350~510 ReH: ≥245 ≥24
100<t≤150 350~510 ReH: ≥240 ≥24
specimen 20°C long. ≥63
tr. ≥40
specimen 0°C long. ≥55
tr. ≥34
specimen -10°C long. ≥51
tr. ≥30
specimen -20°C long. ≥47
tr. ≥27
specimen -30°C long. ≥40
tr. ≥23
specimen -40°C long. ≥31
tr. ≥20
specimen -50°C long. ≥27
tr. ≥16
S275ML Corresponding Standards(Same grade name, different standards)