Grade NiMo28
Germany W-Nr. 2.4617
Corresponding Standard DIN 17750-2002
Wrought nickel and nickel alloy sheet,plate and strip Requirements and testing
Classification Special Alloy Steel
Properties Corrosion Resistance
Density 9.2 g/cm3
NiMo28 Chemical Element Composition Content (%)
Component Fe C Si Mn P S Cr Cu Mo Co More
Minimum Value - - - - - - - - 26 - Ni:余量
Maximum Value 2 0.01 0.08 1 0.025 0.015 1 0.5 30 1
NiMo28 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Strip steel; 0.2<t≤2.5 Solid Solution Treatment (F75) ≥750 ≥340 ≥40 ≤240
Thin Sheet and Thick Plate; 1<t≤65 Solid Solution Treatment (F75) ≥750 ≥340 ≥40 ≤240
Approximate Comparison Table corrosion-resistant alloy
China United States Germany United Kingdom
GB ISC Commercial Grade UNS DIN EN/DIN W-Nr. BS EN/BS
NS 3202
(NS 322)
(00Ni70Mo28)
H 01665
H 03202
Hastelloy B -2 N 10665 NiMo 28
Nimofer 6928
2.4617 NA 44

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!