Grade 08
China ISC U20082
Corresponding Standard GB /T 699-1999
Quality Carbon Structural Steels
Classification Carbon Steel
Properties Low-Temperature Toughness
08 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu
Minimum Value 0.05 0.17 0.35 - - - - -
Maximum Value 0.11 0.37 0.65 0.035 0.035 0.1 0.3 0.25
① The grades listed in the table are of high quality steel. High quality steel, in the grade suffix A, the last digit of the unified digital code is changed to 3; Super high quality steel, in the grade suffix E, the last digit of the unified digital code is changed to 6; The rimming steel, grade suffix F, the last digit of the unified digital code is changed to 0; Semi-killed steel, grade suffix b, unified number code last digit is 1
qulity steel P≤0.035%,S≤0.035%
high qulity steel P≤0.035%,S≤0.035%
speicial high qulity steel P≤0.025%,S≤0.020%
② 08 steel with aluminum deoxidation smelting killed steel, the lower limit of manganese content is 0.25%, silicon content is not more than 0.03%, aluminum content is 0.02%~0.07%, this time the steel grade is 08Al
③ Upon agreement between supply and demand parties, 08~25 steel can be supplied as semi-killed steel with silicon content not exceeding 0.17%, with the grade designations of 08b~25b.
④ Steel produced from scrap metal may have a copper content of no more than 0.30%; the copper content in steel for hot-pressure processing should not exceed 0.20%.
⑤ The silicon content of the rimming steels which used for cold pressing shall be not more
than 0.03%.
⑥ Steel produced by oxygen converter process should have a nitrogen content of no more than 0.008%.
08 Mechanical Properties
diameter(thickness)
d
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
d=25 (Sample size) Normalizing ≥325 ≥195 ≥33 ≥60 Untreated
≤131
① For steel with a diameter or thickness of less than 25mm, heat treatment is performed on a sample blank with the same cross-section size as the finished product
② Table normalizing recommended holding time is not less than 30min, air cooling; The recommended holding time for quenching is not less than 30min,70, 80 and 85 steel oil cooling, and the other steel water cooling; The recommended holding time for tempering is not less than 1h.
1 Approximate Comparison Table High-Quality Carbon Structural Steel
China United States France Russia United Kingdom
GB ISC ASTM/AISI UNS NF EN/NF GOST BS EN/BS
08 U20082 1008 G10080 XC6 08 040A04
050A04
2 Approximate Comparison Table High-Quality Carbon Structural Steel
China Japan United States International Organization for Standardization Germany France European Standard Russia Sweden United Kingdom
GB JIS SAE ISO DIN EN/DIN NF EN/NF EN Numerical Grade GOST SS BS EN/BS
08
08F
SPCC 1008
1010
Cr01
CR22
FeP01
St12
C
F12
FeP01
DC01
FeP01
1.0330 08kp
08ps
1142 CR4
FeP01
3 Approximate Comparison Table High-Quality Carbon Structural Steel
China Japan United States International Organization for Standardization European Standard
GB JIS ASTM/AISI ISO EN
GB/T 699-2015
08
JIS G4051:2005
JIS G3506:2004
S10C
ASTM A29/A29M:2005
1008
ISO 683-18:1996
C10
EN 10083-1:1991+A1:1996
EN 10084:1998
C10E
4 Approximate Comparison Table High-Quality Carbon Structural Steel
China Japan United States European Standard Russia
GB JIS ASTM/AISI EN Numerical Grade GOST
08 SPHE,S10C 1008 DC01
DC03
1.0330
1.0347
08
5 Approximate Comparison Table High-Quality Carbon Structural Steel
China Japan United Kingdom
GB JIS BS EN/BS
GB/T 699-1999
08
JIS G
S9CK
BS
040A04
050A04
08 Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!