Grade 25
China ISC U20252
Other Names
Corresponding Standard GB /T 699-1999
Quality Carbon Structural Steels
Classification Carbon Steel
Properties Impact Toughness Forgability Weldability
25 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu
Minimum Value 0.22 0.17 0.5 - - - - -
Maximum Value 0.29 0.37 0.8 0.035 0.035 0.25 0.3 0.25
① The grades listed in the table are of high quality steel. High quality steel, in the grade suffix A, the last digit of the unified digital code is changed to 3; Super high quality steel, in the grade suffix E, the last digit of the unified digital code is changed to 6; The rimming steel, grade suffix F, the last digit of the unified digital code is changed to 0; Semi-killed steel, grade suffix b, unified number code last digit is 1
qulity steel P≤0.035%,S≤0.035%
high qulity steel P≤0.035%,S≤0.035%
speicial high qulity steel P≤0.025%,S≤0.020%
② 08 steel with aluminum deoxidation smelting killed steel, the lower limit of manganese content is 0.25%, silicon content is not more than 0.03%, aluminum content is 0.02%~0.07%, this time the steel grade is 08Al
③ Upon agreement between supply and demand parties, 08~25 steel can be supplied as semi-killed steel with silicon content not exceeding 0.17%, with the grade designations of 08b~25b.
④ Steel produced from scrap metal may have a copper content of no more than 0.30%; the copper content in steel for hot-pressure processing should not exceed 0.20%.
⑤ The silicon content of the rimming steels which used for cold pressing shall be not more
than 0.03%.
⑥ Steel produced by oxygen converter process should have a nitrogen content of no more than 0.008%.
25 Mechanical Properties
diameter(thickness)
d
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
d=25 (sample diameter) Normalizing or Quenching and Tempering ≥450 ≥275 ≥23 Unprocessed Steel
≤170
① For steel with a diameter or thickness of less than 25mm, heat treatment is performed on a sample blank with the same cross-section size as the finished product
② Table normalizing recommended holding time is not less than 30min, air cooling; The recommended holding time for quenching is not less than 30min,70, 80 and 85 steel oil cooling, and the other steel water cooling; The recommended holding time for tempering is not less than 1h.
1 Approximate Comparison Table
China Taiwan, China Japan South Korea United States International Organization for Standardization Germany France Russia United Kingdom
GB ISC CNS JIS KS ASTM/AISI UNS ISO DIN EN/DIN W-Nr. NF EN/NF GOST BS EN/BS
25 U20252 S25C S25C SM25C 1025 G10250 C25E4 C25E
Ck25
1.1158 C25E
XC25
25 C25E
070M26
2 Approximate Comparison Table
China Japan International Organization for Standardization
GB JIS ISO
25 S25C C25
3 Approximate Comparison Table
China Japan International Organization for Standardization European Standard
GB JIS ISO EN Numerical Grade
25 S25C C25E C22E 1.1151
4 Approximate Comparison Table
China Japan United States International Organization for Standardization France Russia United Kingdom
GB JIS ASTM/AISI ISO NF EN/NF GOST BS EN/BS
GB/T 699-1999
25
S25C 1025 ISO 630-1:1987
C25
C25E4
C25M2
C25
XC25
25 060A25
070A26

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!