Grade SUS405TB
Corresponding Standard JIS G 3463-2019
Stainless steel boiler and heat exchanger tubes
Classification Ferritic Stainless Steel
SUS405TB Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Al
Minimum Value - - - - - 11.5 - 0.1
Maximum Value 0.08 1 1 0.04 0.03 14.5 0.6 0.3
SUS405TB Mechanical Properties
No.12 test piece Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
1<t≤2 ≥11
2<t≤3 ≥12
3<t≤4 ≥14
4<t≤5 ≥16
5<t≤6 ≥17
6<t≤7 ≥18
7<t<8 ≥20
d<10mm(No.11 test piece) ≥410 ≥205 ≥12
10≤d<20mm(No.11 test piece) ≥410 ≥205 ≥15
d≥20mm(No.11 and test piece No.12) ≥410 ≥205 ≥20