Grade C2801
Other Names
Corresponding Standard JIS H 3100-2018
Copper and copper alloy sheets, plates and strips
Classification Copper and Copper Alloys
Properties Strength Machinability
C2801 Chemical Element Composition Content (%)
Component Fe Cu Pb More
Minimum Value - 59 - Zn:余量
Maximum Value 0.07 62 0.1
C2801 Mechanical Properties
condition Mark
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Plate (P), Strip (R, RS); 0.3≤t≤1 C2801 P-O,C2801 R-O,C2801 RS-O Annealing (O) ≥325 ≥35 -
Plate (P); 1<t≤30 C2801 P-O Annealing (O) ≥325 ≥40 -
Strip (R, RS); 1<t≤3 C2801 R-O,C2801 RS-O Annealing (O) ≥325 ≥40 -
Plate (P); 0.3≤t≤30 C2801 P-1/4H 1/4 Hard (1/4H) 355~440 ≥25 HV
85~145
Strip (R, RS); 0.3≤t≤3 C2801 R-1/4H,C2801 RS-1/4H 1/4 Hard (1/4H) 355~440 ≥25 85~145
Plates (P); 0.3≤t≤20 C2801 P-1/2H 1/2 Hard (1/2H) 410~490 ≥15 105~160
Strip (R, RS); 0.3≤t≤3 C2801 R-1/2H,C2801 RS-1/2H 1/2 Hard (1/2H) 410~490 ≥15 105~160
Sheet (P); 0.3≤t≤10 C2801 P-H Hard (H) ≥470 - ≥130
Strip (R, RS); 0.3≤t≤3 C2801 R-H,C2801 RS-H Hard (H) ≥470 - ≥130
Approximate Comparison Table Cupper and cupper alloy
Japan United States International Organization for Standardization Germany France European Standard Russia United Kingdom
JIS UNS ISO DIN EN/DIN W-Nr. NF EN/NF EN Numerical Grade GOST BS EN/BS
C2801 C28000 CuZn40 CuZn40 2.0360 CuZn40 CuZn40 CW509L L60 CZ109