Grade 3J53
Corresponding Standard GB /T 34471.2-2017
Elastic Alloys-Part 2: Constant Elastic Alloys
Classification Alloy Steel
Density 8 g/cm3
3J53 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Ti Al More
Minimum Value - - - - - 5.2 41.5 2.3 0.5 Fe:余量
Maximum Value 0.03 0.8 0.8 0.02 0.02 5.8 43 2.7 0.8
3J53 Mechanical Properties
condition Mark
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Strip -(Grade D); 0.1<d≤3.5 3J53-D-S Solution treatment/soft condition (S)* ≤882 Measured
Wire Material - (Grade C); 0.1<d≤5 3J53-C-WCD Cold drawing / cold drawing (WCD)* ≥931
Wire Rod - (Grade C); 0.5<d≤5 3J53-C-WCD Cold drawn/cold pulled (WCD)** ≥1372 ≥5
Strip-(Grade D); 0.1<d<0.2 3J53-D-S Solution heat treatment/soft state (S)** ≥1078
Strip -(D grade); 0.2≤d≤3.5 3J53-D-S Solution heat treatment/soft state (S)** ≥1078 ≥686 ≥8
Strip-(Grade C); 0.1<d<0.2 3J53-C-WCR Cold rolled (WCR)** ≥1225
Strip -(C grade); 0.2≤d≤3.5 3J53-C-WCR Cold rolled (WCR)** ≥1225 ≥882 ≥5
Bar - (Grade C); 3≤d≤18 3J53-C-WCD Cold drawn/cold pulled (WCD)** ≥1323 ≥1138 ≥5
Bar, Plate - (Grade D); 6≤d<25 3J53-D-WHR/WHF Hot rolling (forging) (WHR/WHF)** ≥1078 ≥621 ≥10
Bar, Plate - (Grade D); d≥25 3J53-D-WHR/WHF Hot rolling (forging) (WHR/WHF)** ≥1078 ≥621 ≥8
Cold Rolled Sheet, Strip Cold processing + Aging*** 1470 HV
420
Approximate Comparison Table Elastic Alloy
China United States Germany France Russia United Kingdom
GB ASTM W-Nr. NF EN/NF GOST BS EN/BS
3J53
(Ni42CrTi)
Ni-Spand Ni-Spand Elinvax 41НХТ Ni-Spand
3J53 Corresponding Standards(Same grade name, different standards)