USA UNS S31651
ASTM
Specification or Grade
316N
Corresponding Standard ASTM A276/A276M-2017
Standard Specification for Stainless Steel Bars and Shapes
Classification Austenitic Stainless Steel
Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo N
Minimum Value - - - - - 16 10 2 0.1
Maximum Value 0.08 1 2 0.045 0.03 18 14 3 0.16
Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
all Annealing - Hot or Cold Precision Rolling (A) ≥550 ≥240 ≥30
≤19.05 Relatively Strict Cold Working (B) ≥860 ≥690 ≥12 ≥35
>19.05~25.4 Relatively Strict Cold Working (B) ≥795 ≥550 ≥15 ≥35
>25.4~31.75 Relatively Strict Cold Working (B) ≥725 ≥450 ≥20 ≥35
>31.75~38.1 Relatively Strict Cold Working (B) ≥690 ≥345 ≥24 ≥45
>38.1~44.45 Relatively Strict Cold Working (B) ≥655 ≥310 ≥28 ≥45
≤50.8 Work Hardening - Relatively Light Cold Working (S) ≥650 ≥515 ≥25 ≥40
>50.8~63.5 Work Hardening - Relatively Light Cold Working (S) ≥620 ≥450 ≥30 ≥40
>63.5~76.2 Work Hardening - Relatively Light Cold Working (S) ≥550 ≥380 ≥30 ≥40
1 Approximate Comparison Table Austenitic Stainless Steel
China Taiwan, China Japan South Korea United States Germany
GB ISC CNS JIS KS ASTM UNS DIN EN/DIN W-Nr.
06Cr17Ni12Mo2N
(0Cr17Ni12Mo2N)
S31658 316N SUS 316N STS 316N 316N S31651 X2CrNiMoN17-11-2 1.4406
2 Approximate Comparison Table Austenitic Stainless Steel
China Japan United States International Organization for Standardization European Standard
GB ISC JIS UNS ISO Numerical Grade Numerical Grade
06Cr17Ni12Mo2N S31658 SUS316N S31651 X6CrNiMoN17-12-3 4495-316-51-J (1.4495)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!