3.7164
Corresponding Standard WL 3.7164-2(1990)
Aerospace; titanium alloy with approx. 6Al-4V; bars and forgings
Classification Titanium and Titanium Alloys
Density 4.4 g/cm3
Chemical Element Composition Content (%)
Component Fe C N V Al H O Other Total More
Minimum Value - - - 3.5 5.5 - - - Ti:余量
Maximum Value 0.3 0.08 0.05 4.5 6.75 0.0125 0.2 0.4
"Other individual elements or other totals": The chemical composition includes elements not specified in the table. Analysis should only be conducted if these elements are suspected to be present, or if routine analysis suggests that their content may exceed the prescribed limits.
Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Forging, Bar; d≤80; Longitudinal Annealing ≥900 ≥830 ≥10 ≥25
Forging, Bar; 80<d≤150; Longitudinal Annealing ≥900 ≥830 ≥8 ≥20
Forging, Bar; d≤13; Longitudinal Solution heat treatment + aging ≥1100 ≥1030 ≥8 ≥15
Forging, Bar; 13<d≤25; Longitudinal Solution heat treatment + aging ≥1070 ≥1000 ≥8 ≥15

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!