Grade Z 7 CND 17-12-02
Other Names
Corresponding Standard NF A 35-574-1990
Iron and steel. Stainless steel for general purposes. Semi - finished products, bars and wire rod
Classification Austenitic Stainless Steel
Properties Corrosion Resistance
Density 7.95 g/cm3
Z 7 CND 17-12-02 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo
Minimum Value - - - - - 16.5 10.5 2
Maximum Value 0.07 0.75 2 0.04 0.015 18.5 12.5 2.5
Z 7 CND 17-12-02 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
For Machined Bar, Wire rod Softening Treatment 530~730 ≥200 ≥40 ≥110
Used for Forging and Re-rolling Semi-finished Products - - - - ≤215 -
Semi-finished products for hot-spinning - - - - ≤215 -
Wire rod for drawing or forming Softening Treatment ≤640 - - -
bar, rod, semi-finished product Cold working hardening (E700) 700~850 ≥350 ≥20 - -
bar, rod, semi-finished product Cold working hardening (E800) 800~1000 ≥500 ≥12 - -
Approximate Comparison Table Austenitic Stainless Steel
China Japan United States Germany France European Standard Russia Sweden United Kingdom
GB JIS ASTM DIN EN/DIN NF EN/NF EN Numerical Grade GOST SS BS EN/BS
0Cr17Ni12Mo2 SUS316 316 X5CrNiMo17-12-2 Z6CND17-11
Z7CND17-11-02
Z7CND17-12-02
X5CrNiMo17-12-2 1.4401 08KH16N11M3 2347 316S31

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!