Grade 325S31
Corresponding Standard BS 970-3-1991
Specification for wrought steel for machanical and allied engineering purposes part 3:bright bars for general engineering purposes
Classification Austenitic Stainless Steel
Properties Corrosion Resistance
325S31 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu * Mo * Nb * More
Minimum Value - - - - 0.15 17 8 - - - Ti:5C~0.9
Maximum Value 0.12 1 2 0.045 0.35 19 11 0.7 1 0.2
• For older grades of stainless steel, see Table 2 of standard BS 970-4-1970
325S31 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Bars; d≤19 Cold Drawing ≥865 ≥695 ≥12
Bars; 19<d≤25 Cold Drawing ≥790 ≥555 ≥15
Bars; 25<d≤32 Cold Drawing ≥725 ≥450 ≥20
Bars; 32<d≤38 Cold Drawing ≥695 ≥340 ≥28
Bars; 38<d≤45 Cold Drawing ≥650 ≥310 ≥28
Bars; d≤19 Annealing Treatment, Final Cold Drawing ≥600 ≥375 ≥15
Bars; d>19 Annealing Treatment, Final Cold Drawing ≥550 ≥325 ≥20
Bars; d<160 Final Softening* ≥510 ≥200 ≥35

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!