Grade NCF750
Corresponding Standard JIS G 4901-2008
Corrosion-Resistant and Heat-Resisting Superalloy Bars
Classification Alloy Steel
Properties Corrosion Resistance
NCF750 Chemical Element Composition Content (%)
Component Fe C Si Mn P S Cr Ni Cu Ti Al More
Minimum Value 5 - - - - - 14 70 - 2.25 0.4 Nb+Ta:0.7~1.2
Maximum Value 9 0.08 0.5 1 0.03 0.015 17 - 0.5 2.75 1
NCF750 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Bars; 2.5<d≤100 Solution (S) - - - ≤320
Bars; 2.5<d≤100 Solution heat treatment + aging (H1) ≥960 ≥615 ≥8 ≥262
Bar; 2.5<d≤60 Solution treatment + aging (H2) ≥1170 ≥795 ≥18 302~363
Bar; 60<d≤100 Solution treatment + aging (H2) ≥1170 ≥795 ≥15 302~363
NCF750 Corresponding Standards(Same grade name, different standards)