USA UNS S46500
Corresponding Standard ASTM A693-2013
Precipitation-Hardening Stainless and Heat-Resisting Steel Plate, Sheet, and Strip
Classification Precipitation-Hardening Stainless Steel
Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo N Ti
Minimum Value - - - - - 11 10.8 0.75 - 1.5
Maximum Value 0.02 0.25 0.25 0.015 0.01 12.5 11.2 1.25 0.01 1.8
Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
t≤3.56 Solid Solution Treatment ≤1105 ≤1035 ≥4 HRC
≤33
t≤3.56 Precipitation Hardening, 482℃ ≥1690 ≥1620 ≥2 HRC
≥48
t≤3.56 Precipitation Hardening, 510℃ ≥1620 ≥1550 ≥3 HRC
≥47
t≤3.56 Precipitation Hardening, 538°C ≥1515 ≥1445 ≥4 HRC
≥45
t≤3.56 Precipitation Hardening, 566°C ≥1380 ≥1275 ≥5 HRC
≥43
t≤3.56 Precipitation Hardening, 593°C ≥1240 ≥1000 ≥6 HRC
≥39

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!