Grade 12NiCr3-2
European Standard Steel Grade 1.5701
Corresponding Standard EN 10263-3-2017
Steel rod, bars and wire for cold heading and cold extrusion Part 3: Technical delivery conditions for steels for case hardening steels
Classification Alloy Steel
12NiCr3-2 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu
Minimum Value 0.09 - 0.3 - - 0.4 0.5 -
Maximum Value 0.15 0.3 0.6 0.025 0.025 0.7 0.8 0.25
12NiCr3-2 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Reduction of Area
ψ
%
Hardness
HBW
Bars; 5<d≤40 Processed to Ferrite-Pearlite Structure and Hardness Range (+FP) 130~180
Bars; 5<d≤40 Spheroidizing (+AC) ≤500 ≥62
Bar, wire; 2<d≤5 Untreated, Cold Drawn, Spheroidizing Treatment (+U+C+AC) ≤500 ≥64
Bar, wire; 5<d≤40 Untreated, Cold Drawn, Spheroidizing Treatment (+U+C+AC) ≤480 ≥64
Bar, wire; 2<d≤5 Untreated, Cold Drawn, Spheroidizing Treatment, and Tempered Rolling (+U+C+AC+LC) ≤540 ≥62
Bar, wire; 5<d≤40 Untreated, Cold Drawn, Spheroidizing Treatment, and Tempered Rolling (+U+C+AC+LC) ≤520 ≥62
Bars, wire; 5<d≤10 Spheroidizing Treatment and Cold Drawing (+AC+C) ≤620 ≥59
Bars, wire; 10<d≤40 Spheroidizing Treatment and Cold Drawing (+AC+C) ≤610 ≥59
Approximate Comparison Table
International Organization for Standardization European Standard
ISO EN Numerical Grade
12NiCr3-2 12NiCr3-2 1.5701
12NiCr3-2 Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!