Grade
18MnB4
European Standard Steel Grade
1.5521
Corresponding Standard
EN 10263-3-2017
Steel rod, bars and wire for cold heading and cold extrusion Part 3: Technical delivery conditions for steels for case hardening steels
Classification
Alloy Steel
18MnB4 Chemical Element Composition Content (%)
Component
C
Si
Mn
P
S
Cu
B
Minimum Value
0.16
-
0.9
-
-
-
0.0008
Maximum Value
0.2
0.3
1.2
0.025
0.025
0.25
0.005
18MnB4 Mechanical Properties
condition
Heat Treatment or Condition
Tensile Strength σb
Mpa
Reduction of Area ψ
%
Bars, rods, wire; 5<d≤40
Untreated (+U)
≤580
≥55
Bars, rods, wire; 5<d≤40
Spheroidizing or Spheroidizing + Rotary Peeling (+AC or +AC+PE)
≤500
≥64
Bars, wire; 5<d≤10
Untreated and Cold Drawn (+U+C)
≤680
≥53
Bars, wire; 10<d≤40
Untreated and Cold Drawn (+U+C)
≤670
≥53
Bar, wire; 2<d≤5
Untreated, Cold Drawn, and Spheroidized (+U+C+AC)
≤500
≥64
Bar, wire; 5<d≤40
Untreated, Cold Drawn, and Spheroidized (+U+C+AC)
≤480
≥64
Bar, wire; 2<d≤5
Untreated, Cold Drawn, Spheroidizing Treatment, and Tempered Rolling (+U+C+AC+LC)
≤540
≥62
Bar, wire; 5<d≤40
Untreated, Cold Drawn, Spheroidizing Treatment, and Tempered Rolling (+U+C+AC+LC)
≤520
≥62
Bars, wire; 5<d≤10
Spheroidizing Treatment and Cold Drawing (+AC+C)
≤600
≥59
Bars, wire; 10<d≤40
Spheroidizing Treatment and Cold Drawing (+AC+C)
≤590
≥59
Approximate Comparison Table Steel for Cold Heading and Cold Extrusion
International Organization for Standardization
European Standard
ISO
EN
Numerical Grade
18MnB4
18MnB4
1.5521
18MnB4 Corresponding Standards(Same grade name, different standards)
Message
I want to correct it
Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!