Grade
18B2
European Standard Steel Grade
1.5503
Corresponding Standard
EN 10263-3-2017
Steel rod, bars and wire for cold heading and cold extrusion Part 3: Technical delivery conditions for steels for case hardening steels
Classification
Alloy Steel
18B2 Chemical Element Composition Content (%)
Component
C
Si
Mn
P
S
Cu
B
Minimum Value
0.16
-
0.6
-
-
-
0.0008
Maximum Value
0.2
0.3
0.8
0.025
0.025
0.25
0.005
18B2 Mechanical Properties
condition
Heat Treatment or Condition
Tensile Strength σb
Mpa
Reduction of Area ψ
%
Bars, rods, wire; 5<d≤40
Untreated (+U)
≤520
≥58
Bars, rods, wire; 5<d≤40
Spheroidizing or Spheroidizing + Rotary Peeling (+AC or +AC+PE)
≤460
≥64
Bars, wire; 5<d≤10
Untreated and Cold Drawn (+U+C)
≤610
≥56
Bars, wire; 10<d≤40
Untreated and Cold Drawn (+U+C)
≤600
≥56
Bar, wire; 2<d≤5
Untreated, Cold Drawn, and Spheroidized (+U+C+AC)
≤450
≥67
Bar, wire; 5<d≤40
Untreated, Cold Drawn, and Spheroidized (+U+C+AC)
≤440
≥67
Bar, wire; 2<d≤5
Untreated, Cold Drawn, Spheroidizing Treatment, and Tempered Rolling (+U+C+AC+LC)
≤490
≥65
Bar, wire; 5<d≤40
Untreated, Cold Drawn, Spheroidizing Treatment, and Tempered Rolling (+U+C+AC+LC)
≤480
≥65
Bars, wire; 5<d≤10
Spheroidizing Treatment and Cold Drawing (+AC+C)
≤550
≥62
Bars, wire; 10<d≤40
Spheroidizing Treatment and Cold Drawing (+AC+C)
≤540
≥62
Approximate Comparison Table
International Organization for Standardization
European Standard
ISO
EN
Numerical Grade
18B2
18B2
1.5503
18B2 Corresponding Standards(Same grade name, different standards)
Message
I want to correct it
Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!