Grade
C17E2C
European Standard Steel Grade
1.1147
Corresponding Standard
EN 10263-3-2017
Steel rod, bars and wire for cold heading and cold extrusion Part 3: Technical delivery conditions for steels for case hardening steels
Classification
Carbon Steel
C17E2C Chemical Element Composition Content (%)
Component
C
Si
Mn
P
S
Cu
Minimum Value
0.15
-
0.6
-
-
-
Maximum Value
0.19
0.3
0.9
0.025
0.025
0.25
C17E2C Mechanical Properties
condition
Heat Treatment or Condition
Tensile Strength σb
Mpa
Reduction of Area ψ
%
Bars, rods, wires; 5<d≤100
Unprocessed or Descaled (+U or +PE)
≤530
≥58
Bars, rods, wires; 5<d≤100
Spheroidizing or Spheroidizing and Peeling (+AC or +AC+PE)
≤450
≥65
Bars, wire; 5<d≤10
Untreated and Cold Drawn (+U+C)
≤630
≥56
Bars, wire; 10<d≤40
Untreated and Cold Drawn (+U+C)
≤620
≥56
Bar, wire; 2<d≤5
Untreated, Cold Drawn, and Spheroidized (+U+C+AC)
≤440
≥67
Bar, wire; 5<d≤40
Untreated, Cold Drawn, and Spheroidized (+U+C+AC)
≤430
≥67
Bar, wire; 2<d≤5
Untreated, Cold Drawn, Spheroidizing Treatment, and Tempered Rolling (+U+C+AC+LC)
≤480
≥65
Bar, wire; 5<d≤40
Untreated, Cold Drawn, Spheroidizing Treatment, and Tempered Rolling (+U+C+AC+LC)
≤470
≥65
Bars, wire; 5<d≤10
Spheroidizing Treatment and Cold Drawing (+AC+C)
≤550
≥62
Bars, wire; 10<d≤40
Spheroidizing Treatment and Cold Drawing (+AC+C)
≤540
≥62
1 Approximate Comparison Table
2 Approximate Comparison Table
3 Approximate Comparison Table Steel for Cold Heading and Cold Extrusion
International Organization for Standardization
European Standard
ISO
EN
Numerical Grade
C17E2C
C17E2C
1.1147
C17E2C Corresponding Standards(Same grade name, different standards)
Message
I want to correct it
Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!