Grade A193 B8N Class 2
USA UNS S30451
Other Names
Corresponding Standard ASTM A193/A193M-2020
Alloy-Steel and Stainless Steel Bolting for High Temperature or High Pressure Service and Other Special Purpose Applications
Classification Austenitic Stainless Steel
Properties Corrosion Resistance Forgability
A193 B8N Class 2 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni N
Minimum Value - - - - - 18 8 0.1
Maximum Value 0.08 1 2 0.045 0.03 20 11 0.16
• The intentional addition of Bi, Se, Te, and Pb is not permitted
A193 B8N Class 2 Mechanical Properties
diameter
d
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
d≤M20 Solid Solution Treatment + Strain Hardening ≥860 ≥690 ≥12 ≥35 ≤321
M20<d≤M24 Solid Solution Treatment + Strain Hardening ≥795 ≥550 ≥15 ≥35 ≤321
M24<d≤M30 Solid Solution Treatment + Strain Hardening ≥725 ≥450 ≥20 ≥35 ≤321
M30<d≤M36 Solid Solution Treatment + Strain Hardening ≥690 ≥345 ≥28 ≥45 ≤321
• d-diameter of bolt, screw, studs, double-end studs, bars and wire.
Approximate Comparison Table
China Taiwan, China Japan South Korea United States International Organization for Standardization European Standard
GB ISC CNS JIS KS ASTM UNS ISO Numerical Grade EN Numerical Grade
06Cr19Ni10N
(0Cr19Ni9N)
S30458 304N1 SUS 304N1
SUS 304N2
STS 304N1 304N S30451 X5CrNiN 19-9 4315-304-51-I X5CrNiN 19-9 1.4315
A193B8NClass2 Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!