Grade X1CrNiSi 18-15-4
European Standard Steel Grade 1.4361
Corresponding Standard EN 10088-3-2014
Stainless steels-Part 3: Technical delivery condition for semi-finished products, bars, rods, wire, sections and bright products of corrosion resisting steels for general purposes
Classification Austenitic Stainless Steel
Properties Corrosion Resistance
Density 7.7 g/cm3
X1CrNiSi 18-15-4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo N
Minimum Value - 3.7 - - - 16.5 14 - -
Maximum Value 0.015 4.5 2 0.025 0.01 18.5 16 0.2 0.1
X1CrNiSi 18-15-4 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
Bar, rod, wire, section, bright products; d≤160 +AT 530~730 ≥210 (long.)
≥40
≤230 (long.)
≥100
Bar, rod, wire, section, bright products; 160<d≤250 +AT 530~730 ≥210 (tr.)
≥30
≤230 (tr.)
≥60
Approximate Comparison Table Austenitic Stainless Steel
International Organization for Standardization European Standard
ISO Numerical Grade Numerical Grade
X1CrNiSi18-15-4 4361-306-00-E 1.4361

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!