Grade X20Cr13
1.4021
Corresponding Standard NF EN 10088-2-2005
Part2:Technical delivery conditions for sheet/plate and strip of corrosion resisting steels for general purposes
Classification Martensitic Stainless Steel
X20Cr13 Chemical Element Composition Content (%)
Component C Si Mn P S Cr
Minimum Value 0.16 - - - - 12
Maximum Value 0.25 1 1.5 0.04 0.015 14
◎ Elements not listed in this table shall not be intentionally added to the steel without the agreement of the purchaser except for finishing the cast. All appropriate precautions are to be taken to avoid the addition of such elements from scrap and other materials used in production which would impair mechanical properties and the suitability of the steel.
X20Cr13 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
Cold-rolled strip steel: T≤3mm +QT - - - HRC:44 to 50 ; HV:440 to 530 -
Cold rolled strip steel: T ≤ 8mm +A ≤700 - ≥ 15① HRB:≤ 95 ; HB/HV:≤ 225 -
Hot rolled strip steel: T ≤ 13.5mm +A ≤700 - ≥ 15① HRB:≤ 95 ; HB/HV:≤ 225 -
Hot-rolled medium and thick plates: T ≤ 75mm② +QT650 650~850 ≥450 ≥ 12① - T >10mm:
by agreement
Hot-rolled medium and thick plates: T ≤ 75mm② +QT750 750~950 ≥550 ≥ 10① - T >10mm:
by agreement
◎ T-thickness;l-longitudinal;t-trasverse
◎ +A=soft annealed;+QT=quenched and tempered;+P=precipitation hardened;+AT=solutiong annealed;+SR=strength relieved
Approximate Comparison Table
China Japan United States Germany France European Standard Russia Sweden United Kingdom
GB JIS ASTM UNS DIN EN/DIN NF EN/NF EN Numerical Grade GOST SS BS EN/BS
20Cr13
2Cr13
X20Cr13