Grade X5CrNiN19-9
1.4315
Corresponding Standard NF EN 10028-7-2000
Flat products made of steels for pressure purposes Part 7: Stainless steels
Classification Austenitic Stainless Steel
X5CrNiN19-9 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni N
Minimum Value - - - - - 18 8 0.12
Maximum Value 0.06 1 2 0.045 0.015 20 11 0.22
◎ Elements not quoted in this table shall not be intentionally added to the steel without the agreement of the purchaser except for finishing the cast. All precautions are to be taken to avoid the addition of such elements from scrap and other materials used in production which would impair mechanical properties and the suitability of the steel.
X5CrNiN19-9 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
C:T ≤ 6 +AT 550~750 Rp0.2:≥290
Rp1.0:≥320
①②
T < 3mm: ≥40
T ≥ 3mm: ≥ 40
②③
20℃:
(l: ≥100;t: ≥60)
-196℃:
(t: ≥60)
H:T ≤ 12 +AT 550~750 Rp0.2:≥270
Rp1.0:≥310
①②
T < 3mm: ≥40
T ≥ 3mm: ≥ 40
②③
20℃:
(l: ≥100;t: ≥60)
-196℃:
(t: ≥60)
P:T ≤ 75 +AT 550~750 Rp0.2:≥270
Rp1.0:≥310
①②
T < 3mm: ≥40
T ≥ 3mm: ≥ 40
②③
20℃:
(l: ≥100;t: ≥60)
-196℃:
(t: ≥60)
Steel: 20℃ ④ - ≥550 Rp0.2:≥270
Rp1.0:≥310
≥40 -
Steel: -80℃ ④ - ≥890 Rp0.2:≥385
Rp1.0:≥455
≥40 -
Steel: -150℃ ④ - ≥1180 Rp0.2:≥450
Rp1.0:≥550
≥35 -
Steel: -196°C ④ - ≥1350 Rp0.2:≥550
Rp1.0:≥650
≥35 -
◎ C-Cold rolled strip;H-Hot rolled strip;P-Hot rolled plate;T-Thickness;t-transverse;l-Longitudinal
◎ +A=annealed;+AT=solution annealed;+QT = quenched and tempered;+RA=recrystallizing annealed condition

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!