Grade C20E2C
Corresponding Standard ISO 4954-1-2024
Steels for cold heading and cold extruding - Technical delivery conditions - Part1: Non-alloy and alloy steels
Classification Carbon Steel
C20E2C Chemical Element Composition Content (%)
Component C Si Mn P S Cu
Minimum Value 0.18 - 0.3 - - -
Maximum Value 0.22 0.3 0.6 0.025 0.025 0.25
C20E2C Mechanical Properties
diameter
d
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Reduction of Area
ψ
%
5<d≤100 +AR or +PE ≤530 ≥58*
5<d≤100 +AC or
+AC+PE
≤470 ≥65
5<d≤10 +AR+C ≤640 ≥56
10<d≤40 ≤630 ≥56
2≤d≤5 +AR+C+AC ≤460 ≥67
5<d≤10 ≤450 ≥67
10<d≤40 ≤450 ≥67
2≤d≤5 +AR+C+AC+LC ≤500 ≥65
5<d≤40 ≤490 ≥65
5<d≤10 +AC+C ≤580 ≥62
10<d≤40 ≤570 ≥62
①+AR=as hot-rolled;+AR or +PE=as hot-rolled or peeled;+AR+C=as hot-rolled+cold drawn;+AR+C+AC=as hot-rolled+cold drawn+spheroidized;+AR+C+AC+LC=as hot-rolled+cold drawn+spheroidized+skin passed;+AC= spheroidized ;+AC or +AC+PE=spheroidized or spheroidized+peeled;+AC+C=spheroidized +cold drawn;+FP=treated to ferrite-pearlite structure and hardness range;+AC+C+AC=spheroidized +cold drawn + spheroidized;+AC+C+AC+LC=spheroidized +cold drawn + spheroidized + skin passed
• Mechanical properties of non-alloy case-hardening steels
* The values are given only for information.
Approximate Comparison Table
International Organization for Standardization European Standard
ISO EN Numerical Grade
C20E2C C20E2C 1.1152
C20E2C Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!