Grade CuNi2Si
Germany W-Nr. CW111C
Corresponding Standard DIN EN 12449-2019
Copper and copper alloys - Seamless, round tubes for general purposes
Classification Copper and Copper Alloys
Density 8.8 g/cm3
CuNi2Si Chemical Element Composition Content (%)
Component Fe Si Mn Ni Pb Other Total More
Minimum Value - 0.4 - 1.6 - - Cu:Rem.
Maximum Value 0.2 0.8 0.1 2.5 0.02 0.3
"Other individual elements or other totals": The chemical composition includes elements not specified in the table. Analysis should only be conducted if these elements are suspected to be present, or if routine analysis suggests that their content may exceed the prescribed limits.
CuNi2Si Mechanical Properties
Wall thickness
t
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Specified Plastic Yield Strength
Rp0.2
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
t≤10 R260 (Solution heat treated) ≥260 ≥60 ≥30
t≤10 H065 (Solution heat treated) 60~90
t≤10 R460 (Solution heat treated and precipitation hardened) ≥460 ≥300 ≥12
t≤10 H150 (Solution heat treated and precipitation hardened) 140~180
t≤10 R380 (Solution heat treated and cold formed) ≥380 ≥260 ≥6
t≤10 H130 (Solution heat treated and cold formed) 120~160
t≤10 R600 (Solution heat treated, cold formed and precipitation hardened) ≥600 ≥480 ≥8
t≤10 H190 (Solution heat treated, cold formed and precipitation hardened) ≥180
Approximate Comparison Table Cupper and cupper alloy
Germany European Standard
DIN EN/DIN W-Nr. EN Numerical Grade
CuNi2Si 2.0855 CuNi2Si CW111C

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!