Grade 4140
Corresponding Standard ASTM A519/A519M-2024
Standard Specification for Seamless Carbon and Alloy Steel Mechanical Tubing
Classification Alloy Steel
4140 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni * Cu * Mo
Minimum Value 0.38 0.15 0.75 - - 0.8 - - 0.15
Maximum Value 0.43 0.35 1 0.04 0.04 1.1 0.25 0.35 0.25
4140 Mechanical Properties
condition Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
HR-Hot rolled 825 620 15 HRB
100
SR-Stress Relieved 825 690 10 HRB
100
A-Annealed 550 415 25 HRB
85
N-Normalized 825 620 20 HRB
100
1 Approximate Comparison Table Alloy Steel for Quenching and Tempering
United States International Organization for Standardization Germany France European Standard
ASTM ISO DIN EN/DIN NF EN/NF EN Numerical Grade
4140 42CrMoS4 42CrMoS4 42CD4u 42CrMoS4 1.7227
2 Approximate Comparison Table Structural Alloy Steel
China Japan United States International Organization for Standardization Germany France European Standard Russia Sweden United Kingdom
GB JIS ASTM ISO DIN EN/DIN NF EN/NF EN Numerical Grade GOST SS BS EN/BS
42CrMo SCM440H 4140
4142
42CrMo4 42CrMo4 42CD4 42CrMo4 1.7225 35KHM
38KHM
2244 708M40
CFS11
3 Approximate Comparison Table Structural Alloy Steel
Japan United States
JIS ASTM AISI
SNB7 A193 B7 4140
4142
4145
4 Approximate Comparison Table Steel for Cold Heading and Cold Extrusion
China Japan United States International Organization for Standardization European Standard
GB JIS ASTM ISO EN
ML40CrMo SCM440 4140 42CrMo4 42CrMo4
5 Approximate Comparison Table Steel for Cold Heading and Cold Extrusion
China Japan United States International Organization for Standardization European Standard
YB GB JIS ASTM ISO EN
QML40CrMo ML40CrMo SCM440 4140 42CrMo4 42CrMo4

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!