Grade 022Cr19Ni10N
China ISC S30453
Corresponding Standard GB /T 713.7-2023
Steel Plate,Sheet and Strip for Pressure Equipments Part7:Stainless Steel and Heat Resisting Steel
Classification Austenitic Stainless Steel
Properties Corrosion Resistance
Density 7.93 g/cm3
022Cr19Ni10N Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni N
Minimum Value - - - - - 18 8 0.1
Maximum Value 0.03 1 2 0.035 0.015 20 11 0.16
022Cr19Ni10N Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Specified Plastic Yield Strength
Rp0.2
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
Solutioon treatment ≥515 Rp0.2: ≥205
Rp1.0: ≥310
≥40 HBW: ≤201
HRB: ≤92
HV: ≤220
20°C:
Long: ≥100
tr: ≥60
-196°C:
tr: ≥60
Approximate Comparison Table Austenitic Stainless Steel
China Taiwan, China Japan South Korea United States International Organization for Standardization Germany France European Standard Sweden United Kingdom
GB ISC CNS JIS KS ASTM UNS ISO DIN EN/DIN W-Nr. NF EN/NF EN Numerical Grade SS BS EN/BS
022Cr19Ni10N
(00Cr18Ni10N)
S30453 304LN SUS 304LN STS 304LN 304LN S30453 X2CrNiN 18-9
X2CrNiN18-10
X2CrNiN 18-10 1.4311 Z2CN 18-1Az
Z3CN18-10Az
X2CrNiN 18-10 1.4311 2371 304S62
304S61

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!