Grade 022Cr25Ni7Mo4N
China ISC S25073
Other Names
Old Grade
Corresponding Standard GB /T 21833-2008
Austenitic-Ferritic (duplex) grade stainless steel seamless tubes and pipes
Classification Duplex Stainless Steel
Properties Corrosion Resistance Machinability Weldability
Density 7.8 g/cm3
022Cr25Ni7Mo4N Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo N
Minimum Value - - - - - 24 6 - 3 0.24
Maximum Value 0.03 0.8 1.2 0.035 0.02 26 8 0.5 5 0.32
022Cr25Ni7Mo4N Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
1025~1125°C, Rapid cooling ≥800 ≥450 ≥15 ≤300
1 Approximate Comparison Table Austenitic-Ferritic Stainless Steel
China Japan United States International Organization for Standardization Germany European Standard
GB ISC JIS ASTM UNS ISO Numerical Grade DIN EN/DIN W-Nr. EN Numerical Grade
022Cr25Ni7Mo4N S25073 UR 47N+ 2507 S32750 X2CrNiMoN25-7-4 4410-327-50-E X2CrNiMoN25-7-4 1.4410 X2CrNiMoN25-7-4 1.4410
2 Approximate Comparison Table Austenitic-Ferritic Stainless Steel
China United States International Organization for Standardization United Kingdom
GB ISC AISI UNS ISO Numerical Grade BS EN/BS
022Cr25Ni7Mo4N
(GB/T 39033)
S25073 2507 S32750
(ASTM A595-16)
X2CrNiMoN25-7-4
(ISO 15510:2014)
4410-327-50-E X2CrNiMoN25-7-4/1.4410
(BS EN 10088-3:2014)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!